SKH55 HSS bar is a cobalt-alloyed high-speed tool steel, manufactured using a carefully controlled process to ensure an optimal structure with fine carbide size and distribution. This steel is designed to offer excellent hardness, wear resistance, and high red hardness, making it ideal for demanding cutting and machining applications. Its unique manufacturing process enhances its performance and longevity in high-temperature environments, making it a reliable choice for high-performance tooling.
| ZEICIN Grade | GB | ISO | JIS | DIN | AISI |
| SKH55 | W6Mo5Cr4V2Co5 | HS6-5-2-5 | SKH55 | 1.3243/S6525 | M35 |
| C | Mn | P | S | Si | Cr | Mo | V | Co | W |
| 0.87-0.95 | 0.15-0.40 | ≤0.03 | ≤0.03 | 0.20-0.45 | 3.80-4.50 | 4.70-5.20 | 1.70-2.10 | 4.50-5.00 | 5.90-6.70 |
Heat Treatment of SKH55 High-Speed Steel
| Process | Temperature | Procedure | Hardness |
|---|---|---|---|
| Forging | 450-500°C (Preheat), 950-1100°C (Forging) | Preheat and forge, avoiding temperatures below 950°C. | |
| Annealing | 850°C | Heat to 850°C, hold for 1 hour per 25mm thickness, cool slowly. | Max Brinell 260 |
| Stress Relieving | 600-700°C | Heat to 600-700°C, soak for 2 hours, cool slowly. | |
| Hardening | 1050-1250°C | Preheat and heat to 1050-1250°C, then quench. | |
| Tempering | 510-620°C | Triple tempering, hold for 2 hours per cycle. | 67 HRc (540°C), 66 HRc (560°C), 65 HRc (580°C) |